WOOD LAMINATING / BOWMAKING EA-40® has been used for many years for laminating fine woods. It is preferred by bow makers around the world and offers longevity, flexibility and memory required for making award winning performance bows. Suggested laminating procedure; 1. Plane or lightly sand all surfaces to be laminated with 120 grit sand paper 2. Blow off dust with compressed air and wipe all surfaces clean using acetone (Warning – acetone is flammable. Follow acetone manufacturer procedures for handling). Let acetone evaporate for 10 minutes. 3. Mix and apply EA-40® as directed between layers of laminate to sanded surfaces using a brush. 4. Carefully clamp laminated pieces together applying even pressure. 5. Place in oven and use the following step-cure schedule: Temperature Duration 120°F / 48°C 2 hours 150°F / 65°C 2 hours 185°F / 85°C 2 hours Important; Let cool for at least 6 hours to room temperature before releasing clamps or handling.